User Manual
ionTig 200 Pulse PFC
Copyright © Mundaka Welding & Gases, Inc.
24
TIG of stainless steel (single run welding)
Workpiece
thickness
/mm
Joint form
tungsten
electrode
diameter/mm
welding wire
diameter/mm
Argon gas
flow rate/
L·min
-1
welding
current
(DCEP)
Welding
speed/
cm·min
-1
0.8
Butt joint
1.0
1.6
5
20~50
66
1.0
Butt joint
1.6
1.6
5
50~80
56
1.5
Butt joint
1.6
1.6
7
65~105
30
1.5
Corner joint
1.6
1.6
7
75~125
25
2.4
Butt joint
1.6
2.4
7
85~125
30
2.4
Corner joint
1.6
2.4
7
95~135
25
3.2
Butt joint
1.6
2.4
7
100~135
30
3.2
Corner joint
1.6
2.4
7
115~145
25
4.8
Butt joint
2.4
3.2
8
150~225
25
4.8
Corner joint
3.2
3.2
9
175~250
20
Notice: the above parameters originate from《Welding Dictionary》P150, Volume 1 of Edition 2.
Parameters of piping back sealing welding for mild steel(DCEP)
Piping
diameterΦ/mm
Tungsten
electrode
diameter/mm
Gas nozzle
diameter/mm
Welding wire
diameter/mm
Welding
current/A
Arc
voltage/V
Argon
flow rate
/ L·min
-1
Welding
rate
/ cm·min
-1
38
2.0
8
2
75~90
11~13
6~8
4~5
42
2.0
8
2
75~95
11~13
6~8
4~5
60
2.0
8
2
75~100
11~13
7~9
4~5
76
2.5
8~10
2.5
80~105
14~16
8~10
4~5
108
2.5
8~10
2.5
90~110
14~16
9~11
5~6
133
2.5
8~10
2.5
90~115
14~16
10~12
5~6
159
2.5
8~10
2.5
95~120
14~16
11~13
5~6
219
2.5
8~10
2.5
100~
120
14~16
12~14
5~6