Specifications
15BOC Smootharc Advance MIG 200C/275C/275R/350R Operating manual
Argoshield Heavy
Indicative
Welding Parameters Dip Transfer Spray Transfer
Material thickness (mm) 10 12+ 10 12+
Welding position
Horizontal/
Vertical
Horizontal/
Vertical
Horizontal Horizontal
Wire diameter (mm)
1.2 1.2 1.2 1.2
Current (amps)
140–160 140–160 240–260 290–330
Voltage (volts)
17–18 17–18 27–29 28–31
Wire feed speed (m/min)
3.2–4.0 3.2–4.0 7.0–8.0 10.0–12.0
Gas rate flow (L/min)
18 18 18 18
Travel speed (mm/min)
300–450 300–450 400–480 370–440
Argoshield 52 (Aus) or Argoshield FCW (NZ)
Indicative
Welding Parameters Metal Cored Wires Flux Cored Wires
Material thickness (mm) 10 12 20 12 12 20 20
Welding position
Horizontal Horizontal Horizontal Horizontal Vertical Horizontal Vertical
Wire diameter (mm)
1.2 1.2 1.6 1.2 1.2 1.6 1.6
Current (amps)
200–250 300–350 300–400 200–250 175–200 350–400 200–250
Voltage (volts)
27–29 31–34 30–32 25–28 24–25 29–32 24–26
Wire feed speed (m/min)
6.9–10.0 13.2–16.3 5.6–8.4 9.1–13.1 7.5–9.1 8.7–11.2 4.1–5.3
Gas rate flow (L/min)
18 18 18 18 15 18 15
Travel speed (mm/min)
380–550 380–550 350–450 200–300 150–250 300–400 150–200
Stainshield (Aus) or Stainshield MIG (NZ)
Indicative
Welding Parameters Dip Transfer Spray Transfer
Material thickness (mm) 4 6 8 4 6 10
Welding position
Horizontal /
Vertical
Horizontal /
Vertical
Horizontal /
Vertical
Horizontal Horizontal Horizontal
Wire diameter (mm)
0.9–1.0 0.9–1.0 0.9–1.0 1.0 1.2 1.2
Current (amps)
100–125 120–150 120–150 180–220 260–280 260–310
Voltage (volts)
17–19 18–20 18–20 24–28 26–30 28–32
Wire feed speed (m/min)
5.0–6.5 6.0–7.5 6.0–8.0 7.0–9.0 8.0–10.0 9.0–11.0
Gas rate flow (L/min)
15 15 18 18 18 18
Travel speed (mm/min)
400–600 280–500 280–450 350–450 380–460 320–450