Information

Product Test
3. POLYETHYLENE
Diameter: 1 inch
- 5 samples of tubing
- Method according to the ISO 3795 / SAE J369 (Max burn rate 100 mm/min)
Sample 1 Sample 2 Sample 3 Sample 4 Sample 5 Average
68 mm/min 79.5 mm/min 70.2 mm/min 67.3 mm/min 75.8 mm/min 72.1 mm/min
4. HEAT STABILIZED NYLON
Diameter: 1 inch
- 5 samples of tubing
- Method according to the ISO 3795 / SAE J369 (Max burn rate 100 mm/min)
Sample 1 Sample 2 Sample 3 Sample 4 Sample 5 Average
49 mm/min 82 mm/min 65 mm/min 60 mm/min 63.6 mm/min 63.9 mm/min
This document belongs to Panduit. It cannot be communicated or reproduced without Panduit’s authorization.
Page 2 of 2 1/28/2010